What process is chip underfill dispensing?

Take apart a manual machine or a laptop; under the black chips on the main board hides a layer of invisible glue. This glue is underfill, it isChip packaging stagea key process that determines product life. What the dispensing industry calls ”High-precision dispensing”, a large part of the demand comes from this process.

I. What problem does underfill solve

Flip-chip, BGA and such packages solder the chip to the substrate via bottom solder balls or bumps. The chip and substrate have very different thermal-expansion coefficients; the product repeatedly powers on/off, heats/cools, the joint is repeatedly pulled, over time metal fatigue cracks, the equipment shows false solder, dead machine. High-reliability products-automotive chips, processors, power devices-basically all require underfill.

底部填充工艺,high precisiondispensing,底部填充流程

II. Five-step process flow

The industry-standard underfill process is divided into five steps.

Step 1 Cleaning: use IPA to remove flux residue and dust around the chip; residue hinders adhesive flow and adhesion.

Step 2 Preheating: heat the substrate to 40-100℃, reduce adhesive viscosity and speed up subsequent flow.

The third step of dispensing: the needle follows one or two adjacent edges of the chip in an L or U path, squeezing adhesive onto the chip side surfaces.

Step 4 Capillary flow: the adhesive relies on capillary action to flow into the gap under the chip by itself.

Step 5 Curing: enter the curing oven, keep at 120–150℃ for 30–90 minutes.

III. Three parameters most prone to problems

The first is the dispensing path. Do not dispense around all four chip edges-glue from four sides squeezes air trapped in the middle; after curing it is internal voids. Correct: one- or two-side dispensing, letting glue push air to the other side.

Second is the glue amount: aim for the adhesive to flow to the opposite side and overflow the chip edge by 0.5-1mm, 50%-75% overflow; too little leaves voids, too much contaminates nearby pads.Third is the void rate: per IPC-7095, single solder-joint void area not over 25% of joint area, average over all joints not over 15%; exceed means check preheat temperature and path.

IV. Requirements for the dispensing equipment

Underfill belongs toMicro-precision dispensing, and equipment requirements focus on three points.

First is positioning: the needle must hug the chip edge; a deviated start skews the whole glue path. The value of the vision dispensing machine in this process is to first shoot the chip position, then guide the needle along the edge.

The second is dispensing consistency: dispensing valve glue-volume accuracy reaches ±0.001g; jetting valve can inject into hundred-micron narrow gaps; such valve bodies rely on servo-driven platforms to move steadily.

Third is the stroke: Bolli equipment offers a stroke of 300–900mm optional, with multiple chips on a single PCBA completed in one fixturing for continuous underfill.

V. The biggest feature is that it cannot be repaired

Once underfill cures, the chip is basically unrepairable-removal needs local heating plus mechanical force, easily damaging the substrate. So the industry practice: confirm soldering quality before underfill; confirm everything before underfill. This is also its biggest difference from ordinary bonding dispensing: ordinary dispensing wrong dot can be wiped and redone, underfill wrong dot scraps the whole board.

6. Summary

Underfill is a key process for chip reliability; the core flow is cleaning, preheating, one-side dispensing, capillary flow, curing-five steps; the path must never enclose all four sides, the glue amount is based on 50% to 75% overflow to the opposite side, and the void rate is controlled according to IPC-7095 standard;On the equipment side, look at three items: positioning, dispensing consistency and travel, verify with a free sample test before manual operation.